IInconel
Daawaha Heerkulka Sare
◆Inconel600 (N06600) ayaa iska caabin daxalka u leh warbaahinta kala duwan ee daxalka, waxa kale oo uu leeyahay xoog dillaac gurguurta wanaagsan, talinayaa in deegaanka shaqada ka hooseeya 700 ℃.Inta badan waxaa loo isticmaalaa dhinaca wax soo saarka iyo isticmaalka biraha alkali ee daxalka leh, gaar ahaan meelaha lagu isticmaalo sulfides-ka.
Waxqabadka muhiimka ah ee Inconel601 (N06601) waa in uu leeyahay caabbinta oksaydhka iyo iska caabbinta carbonization wanaagsan marka heerkulku uu sarreeyo sida 1180 ° C. Waxaa inta badan loo isticmaalaa qaybaha hababka daaweynta kulaylka, qaybaha nidaamka qiiqa, iyo dib-u-kuliyaha oksijiinta.
◆Inconel625 (N06625Ns336) waxay soo bandhigaysaa iska caabbinta daxalka aad u fiican ee warbaahin badan, iyo 625 annealed annealed low-carbon alloy 625 si ballaaran ayaa loo isticmaalaa warshadaha habka kiimikada, halkaas oo ay la xiriirto biyaha badda oo ay u adkeyso cadaadiska sare ee farsamada.
◆Inconel725 waxay leedahay iska caabin daxalka stress oo xoog leh waxayna ku habboon tahay xirmooyinka tuubooyinka iyo maraakiibta badda.
◆Inconel690 waxa ay leedahay anti-oxidation iyo Properties anti-corrosion, waxayna ku haboon tahay petrochemical, metallurgy, tamarta nukliyeerka, iwm.
Halabuurka kiimikada
Darajo | C | Si | Mn | S | P | Cr | Ni | Fe | Al | Ti | Cu | Mo | Nb | kale |
aan ka weynayn | ||||||||||||||
Inconel600 | 0.15 | 0.5 | 1 | 0.015 | 0.03 | 14 ilaa 17 | saldhig | 6 ilaa 10 | - | - | ≤0.5 | - | - | - |
Inconel601 | 0.1 | 0.5 | 1 | 0.015 | 0.03 | 21 ilaa 25 | saldhig | 10 ilaa 15 | 1. 1.7 | - | ≤1 | - | - | - |
Inconel625 | 0.1 | 0.5 | 0.5 | 0.015 | 0.015 | 20 ilaa 23 | saldhig | ≤5 | ≤0.4 | ≤0.4 | - | 8 ilaa 10 | 3.15-4.15 | Co≤1 |
Inconel725 | 0.03 | 0.2 | 0.35 | 0.01 | 0.015 | 19-22.5 | 55-59 | Hadhi | 0.35 | 1. 1.7 | - | 7-9.5 | 2.75~4 | - |
Inconel690 | 0.05 | 0.5 | 0.5 | 0.015 | 0.03 | 27-31 | ≥58 | 7~11 | - | - | ≤0.5 | - | - | - |
Hantida Alloy ugu yar
Darajo | state alloy | xoogga xajinta RmN/m㎡ | Xoogga Wax-soo-saarka Rp0.2N/m㎡ | Kordhinta sida% | adkaanta Brinell HB |
Inconel600 | Daaweynta xalalka | 550 | 240 | - | ≤195 |
Daaweynta xalalka | 500 | 180 | - | ≤185 | |
Inconel601 | Annealing | 650 | 300 | - | - |
Daaweynta xalalka | 600 | 240 | - | ≤220 | |
Inconel625 | Daaweynta xalalka | 760 | 345 | - | ≤220 |
Inconel725 | Daaweynta xalalka | 790 | 485 | 28 | - |
Inconel690 | Daaweynta xalalka | 780 | 450 | 25 | - |